Rare Earth Oxalate Drying and Calcination: How to Specify the Dryer–Calciner Line

How should you specify drying and calcination for rare earth oxalate? Treat it as two jobs. First remove the free (surface) water from the filtered oxalate cake, then calcine the dry oxalate to oxide at high temperature with enough residence time to reach a low loss on ignition (LOI). One recent Indian public-sector tender shows the scale: it asks for a 200 kg/h electrically heated rotary calciner that turns NdPr oxalate into oxide at 950–1,000°C with about two hours’ residence and an LOI below 0.5%. Most specification mistakes come from mixing up wet feed, dry feed and oxide output, and from ignoring dust, off-gas and iron pick-up.

This guide is for process engineers and project teams planning separation, refining or oxide-to-metal lines. LOI means the percentage weight lost when a sample is heated further. It shows how completely the oxalate has turned into oxide.

Why is rare earth oxide processing on Indian project lists now?

On 26 November 2025 the Union Cabinet approved a ₹7,280 crore Scheme to Promote Manufacturing of Sintered Rare Earth Permanent Magnets. It aims at 6,000 tonnes a year of integrated capacity, covering the conversion of rare earth oxides to metals, metals to alloys and alloys to magnets. BusinessLine reported on 13 August 2026 that 20 bids had been received. Five beneficiaries are envisaged, each with up to 1,200 tonnes a year.

Upstream, IREL (India) Limited’s Rare Earths Division has issued tender IREL/RED/P/26-27/00072 (pre-bid meeting 1 September 2026) for the design, supply and commissioning of an electrically heated tubular rotary calciner for NdPr oxalate. Its data sheet is one of the few public, current specifications for this duty in India, so we use it below as a reference. We quote the tender only as a published specification. It does not mean any supplier has been selected.

What does the oxalate actually contain?

According to the IREL data sheet, the feed is NdPr oxalate, (NdPr)2(C2O4)3·nH2O, from a centrifuge. It is described as follows:

Parameter Value in the tender data sheet
Free moisture 15–20%
Bound moisture (water of crystallisation) 5–10%
Total rare earth oxide (TREO) content 40–45%
Particle size D10 11 µm, D50 53 µm, D90 90.3 µm
Bulk density Feed 0.54 g/cc; product 0.99 g/cc
Calcination 950–1,000°C, normal residence time 2 h
Rated feed / output 200 kg/h feed; approximately 100 kg/h oxide
Product LOI Below 0.5%
Product-contact material SS 310

Three kinds of mass leave the solid. Free water evaporates at modest temperature. Bound water is released as the hydrate breaks down. The oxalate itself then decomposes, releasing carbon monoxide and carbon dioxide (overall, Ln2(C2O4)3 → Ln2O3 + 3CO + 3CO2). Only the first step is ordinary drying. The rest is calcination, and it needs the high temperature and residence time the tender specifies.

Worked example: what does the 200 kg/h feed really carry?

We take the midpoints of the data sheet ranges: 17.5% free moisture, 7.5% bound moisture and 42.5% TREO. We read all three as percentages of the as-received feed. The tender does not state the basis, and that gap matters, as shown below.

Stream (per hour) Calculation Result
Free water 200 × 0.175 35 kg
Bound water 200 × 0.075 15 kg
Oxide in feed (TREO) 200 × 0.425 85 kg (80–90 kg across the stated range)
CO + CO2 and other losses (by difference) 200 − 35 − 15 − 85 about 65 kg

The basis question. If TREO is on the as-received feed, 200 kg/h of feed gives 80–90 kg/h of oxide, not the “approximately 100 kg/h” in the data sheet. The two figures match only if TREO is on a dry basis or the output figure is rounded. A calciner sized on the wrong basis can be 10–20% out on product rate. Before you quote or order, get written answers to three questions: is TREO on a wet or a dry basis, which moisture is guaranteed at the feed hopper, and is the performance test on feed rate or on product rate?

Free-water heat. Heating 35 kg/h of water from about 30°C to 100°C and evaporating it needs roughly 35 × (293 + 2,257) kJ ≈ 89,000 kJ/h, or about 25 kW. That is a theoretical minimum. In an electrically heated calciner, that heat comes from the heater elements and uses up heated length that could otherwise serve calcination. Removing most of the free water in a separate dryer moves this load to cheaper heat (steam or hot air). It also cuts the water vapour in the calciner off-gas.

Pre-drying is not automatically worth it. On a 200 kg/h line, about 25 kW of theoretical electric load may not pay for an extra dryer, conveyor and dust collector, and every transfer of a fine, valuable powder risks losses. On larger lines, or where calciner length is the bottleneck, the case is stronger. Run the numbers with your tariffs and your measured free moisture.

Which equipment does each step?

Step Typical equipment What to watch
Free-water removal (optional pre-dryer) Paddle (indirect), flash, fluid bed or rotary dryer Cake stickiness, fines carry-over, product temperature, contamination
Dehydration and calcination Rotary calciner: indirect electrically heated tube or indirectly fired Zone temperature control, residence time, LOI, off-gas CO
Cooling Cooling zone, rotary or fluid bed cooler Discharge temperature suitable for lined jumbo bags (the IREL data sheet asks for 70°C or below)
Screening and packing Magnetic vibro screen, dust-tight bagging Iron pick-up, dust losses

Indirect heating matters for this product. Direct combustion gases bring contamination and CO2/water loading into a high-purity oxide. That is why the IREL specification uses an electrically heated tube with SS 310 product-contact parts. For the pre-drying step, an indirect paddle dryer handles sticky centrifuge cake with very little gas flow, which keeps dust collection small. Where the cake is free-flowing after the centrifuge, a flash dryer or vibratory fluid bed dryer can be compact. Only trials on your cake can show which works.

What goes wrong in practice?

  • High LOI. Feed rate above design, cold zones or short residence time leave unconverted oxalate or oxycarbonate. Check zone temperatures against the profile, retort speed and slope, and feed-rate control before raising set points.
  • Lumps and wall build-up. Wet cake fed straight into a hot retort can stick and form rings. A lump breaker and controlled screw feeding (both in the IREL scope) help, and so does a steady free-moisture value.
  • Dust losses. With a D50 near 53 µm, fines are carried into the off-gas. At oxide values this high, bag filter catch should normally go back to the product (subject to your quality rules), and the losses should be measured.
  • Off-gas hazards. Oxalate decomposition releases carbon monoxide. The exhaust route, scrubber and room ventilation should be designed for it, and CO monitoring considered where people work. The IREL scope includes a bag filter, scrubber, blower and chimney.
  • Iron and wear contamination. Magnet-grade oxide buyers set tight limits on impurities. Use suitable alloys for product-contact parts, a magnetic screen, and avoid carbon-steel transfer equipment after calcination.

What should go in your enquiry?

  • Oxalate type and chemistry; free and bound moisture, with the measurement method and basis
  • Feed rate and target product rate, stated separately
  • Required LOI and test method (the IREL data sheet describes 2 g calcined at 900°C for 30 minutes, while its scope refers to testing at 1,000°C, so confirm which applies)
  • Particle size, bulk density, and whether the cake is sticky or free-flowing
  • Available utilities: electric load, steam, fuel
  • Product-contact materials, impurity limits and packing format
  • Off-gas treatment and emission requirements at your site

Frequently asked questions

Can one rotary unit both dry and calcine?

Yes. The IREL specification feeds centrifuge oxalate straight into a multi-zone calciner, with preheating zones before the 950–1,000°C zone. A separate pre-dryer is an option for saving energy or capacity, not a requirement.

Is this only for NdPr?

No. Lanthanum, cerium, samarium and other separated rare earths are also precipitated and calcined. The temperatures, residence times and impurity limits differ by element and buyer, so take them from your process licensor or customer specification.

Does drying temperature affect the final oxide?

Calcination conditions largely set particle size and surface area of the oxide. Pre-drying mainly affects lumps, dust and energy. If your downstream metal or magnet process has particle-size limits, test samples from the full drying and calcining sequence, not just the calciner.

About Genex Tech Industries LLP (GTI Group)

Genex Tech Industries LLP (GTI Group) designs and manufactures industrial drying and thermal processing systems. Its rare earth and mineral thermal processing page lists rotary, fluid bed, flash, belt and paddle dryers for rare earth concentrates and other minerals, and rotary calciners for rare earth oxides with a typical operating range of 400°C to 1,200°C. See also GTI’s rotary drum dryer page, this site’s rotary dryer machine page, and our guides on specifying a dryer for specialty and fine chemicals and choosing a dryer for LFP cathode material. The head office is at 10C Middleton Row (Sir William Jones Sarani), Kolkata 700071, India.

Sources and authorship

  • Prime Minister’s Office / Union Cabinet, “Cabinet Approves Rs.7,280 Crore Scheme to Promote Manufacturing of Sintered Rare Earth Permanent Magnets (REPM)”, 26 November 2025.
  • BL New Delhi Bureau, “20 companies bid for ₹7,280-crore rare earth magnet manufacturing scheme”, The Hindu BusinessLine, 13 August 2026.
  • IREL (India) Limited, Rare Earths Division, tender IREL/RED/P/26-27/00072, electrically heated tubular rotary calciner for NdPr oxalate (document published on GeM, August 2026), scope and data sheet.
  • Published thermal processing and dryer pages of Genex Tech Industries LLP (GTI Group) on gtidryers.com.

The worked example is an illustrative calculation using the midpoints of a published specification and stated assumptions. It is not a plant measurement or performance guarantee. Equipment choice for a specific oxalate needs material trials. This article was prepared by the editorial team of Genex Tech Industries LLP (GTI Group) with AI editorial assistance. It has not been reviewed by a named engineer, and no individual is cited as having approved the technical content.